Limits on Unspecified Elements

Copper, max %A
Heat analysis
0.40
Product analysis
0.43
Nickel, max %A
Heat analysis 0.40
Product analysis 0.43
Chromium, max %A,B
Heat analysis 0.30
Product analysis 0.34
Molybdenum, max %A,B
Heat analysis 0.12
Product analysis 0.13
Vanadium, max %C
Heat analysis 0.03
Product analysis 0.04
Columbium, max %C
Heat analysis 0.02
Product analysis 0.03

AThe sum of copper, nickel, chromium, and molybdenum shall not exceed 1.00 % on heat analysis. When one or more of these elements are specified, the sum does not apply, in which case, only the individual limits on the remaining unspecified elements will apply.

BThe sum of chromium and molybdenum shall not exceed 0.32 % on heat analysis. When one or more of these elements are specified, the sum does not apply, in which case, only the individual limits on the remaining unspecified elements will apply.
CBy agreement, the heat analysis limits for vanadium or columbium, or both, may be increased up to 0.10 % and 0.05 %, respectively.

Tensile Requirements

Designation
Yield StrengthA
Tensile Strength
Elongation in 2 in.
[50 mm] min. % for Thickness
Elongation
in 8 in. [200
mm],
min. %
   
Minimum
Maximum
Under 0.270 in.
[7.0 mm]
to 0.145 in.
[3.8 mm]
Under 0.145 in.
[3.8 mm]
to 0.089 in.
[2.2 mm]
Under 0.089 in.
[2.2 mm]
to 0.057 in.
[1.5 mm]
 
 
ksi [MPa]
ksi [MPa]
ksi [MPa]
- - - -
Grade A
25[170] 45[310] 60[415] 26 24 23 20
Grade B
30[205] 50[345] 65[450] 24 22 21 18
Grade C
33[230] 55[380] 70[485] 22 20 19 16
Grade D
35[240] 60[415] 75[515] 20 18 17 14
Grade E
38[260] 65[450] 85[585] 18 16 15 12
Grade F
42[290] 70[485] 90[620] 16 14 13 10
Grade G
45[310] 75[515] 95[655] 16 14 13 10
Grade H
45[310] 75[515] 90[620] 25 24 23 20
AYield strength determined by the 0.2 % offset or 0.5 % extension under load methods.