Heat Treatment and Grain Size RequirementsA
|
Grade
|
UNS
Number
|
Heat Treat Type
|
Austenitizing/
Solutioning/
Stabilizing
Temperature,
min or range °F [°C]
|
Cooling Media
|
Subcritical Annealing
or Tempering
Temperature,
min or range °F [°C]
|
ASTM
Grain Size No.B
|
|
Ferritic Alloy Steels
|
||||||
|
T2
|
K11547
|
full or isothermal
anneal; or
|
- | - | - | - |
|
normalize and
temper; or
|
- | - | - | - | ||
|
subcritical anneal
|
- | - |
1200 to 1350
[650 to 730]
|
- | ||
|
T5
|
K41545
|
full or isothermal
anneal; or
|
- | - | - | - |
|
normalize and
temper
|
- | - |
1250 [675]
|
- | ||
|
T5b
|
K51545
|
full or isothermal
anneal; or
|
- | - | - | - |
|
normalize and
temper
|
- | - |
1250 [675]
|
- | ||
|
T5c
|
K41245
|
subcritical anneal
|
- |
air or furnace
|
1350 [730]C
|
- |
|
T9
|
S50400
|
full or isothermal
anneal; or
|
- | - | - | - |
|
normalize and
temper
|
- | - |
1250 [675]
|
- | ||
|
T11
|
K11597
|
full or isothermal
anneal; or
|
- | - | - | - |
|
normalize and
temper
|
- | - |
1200 [650]
|
- | ||
|
T12
|
K11562
|
full or isothermal
anneal; or
|
- | - | - | - |
|
normalize and
temper; or
|
- | - | - | - | ||
|
subcritical anneal
|
- | - |
1200 to 1350
[650 to 730]
|
- | ||
|
T17
|
K12047
|
full or isothermal
anneal; or
|
- | - | - | - |
|
normalize and
temper
|
- | - |
1200 [650]
|
- | ||
|
T21
|
K31545
|
full or isothermal
anneal; or
|
- | - | - | - |
|
normalize and
temper
|
- | - |
1250 [675]
|
- | ||
|
T22
|
K21590
|
full or isothermal
anneal; or
|
- | - | - | - |
|
normalize and
temper
|
- | - |
1250 [675]
|
- | ||
|
T23
|
K40712
|
normalize and
temper
|
1900–1975
[1040–1080]
|
- |
1350–1470 [730–800]
|
- |
|
T24
|
K30736
|
normalize and
temper
|
1800–1870
[980–1020]
|
D |
1350–1420 [730–770]
|
- |
|
T36
|
K21001
|
normalize and
temper
|
1650 [900]
|
E |
1100 [595]
|
- |
|
T91
|
K90901
|
normalize and
temper
|
1900–1975
[1040–1080]
|
- |
1350–1470 [730–800]
|
- |
|
T92
|
K92460
|
normalize and
temper
|
1900–1975
[1040–1080]
|
- |
1350–1470 [730–800]
|
- |
|
T122
|
K91261
|
normalize and
temper
|
1900–1975
[1040–1080]
|
- |
1350–1470 [730–800]
|
- |
|
T911
|
K91061
|
normalize and
temper
|
1900–1975
[1040–1080]
|
D |
1365–1435
[740–780]
|
- |
AWhere ellipses ({) appear in this table there is no requirement
BASTM Grain Size No. listed, or coarser, unless otherwise indicated.
CApproximately, to achieve properties.
DAccelerated cooling from the normalizing temperature shall be permitted for section thicknesses greater than 3 in. [75 mm].
EAccelerated air cooling or liquid quenching shall be permitted for Class 2.