ApproximateA Relationship Between Shore HFRSc Scleroscope and Diamond Pyramid Hardness for Wrought Hardened Alloy Steel Rolls
NOTE1-This table is recommended for rolls over 6 in. [150 mm] in diameter. There is a tendency for rolls smaller than 6 in. in diameter with the same Vickers hardness to show lower scleroscope readings.
NOTE2- For scleroscope hardness determinations, the calibration to standard reference blocks, and the verification of instrument are a constant necessity. See details recommended in Practice E448.
NOTE3-For Rockwell and Vickers hardness determinations, reference may be made to Test Methods E18 and Test Method E92.
NOTE4-For hardness conversion tables for metals, see Tables E140.
|
Shore HFRSc Scleroscope Hardness
|
Vickers HardnessB
|
Shore HFRSc Scleroscope Hardness
|
Vickers HardnessB
|
| 65 | 420 | 86 | 685 |
| 66 | 432 | 87 | 698 |
| 67 | 445 | 88 | 710 |
| 68 | 457 | 89 | 723 |
| 69 | 470 | 90 | 735 |
| 70 | 482 | 91 | 748 |
| 71 | 495 | 92 | 761 |
| 72 | 508 | 93 | 774 |
| 73 | 520 | 94 | 787 |
| 74 | 533 | 95 | 800 |
| 75 | 545 | 96 | 812 |
| 76 | 558 | 97 | 825 |
| 77 | 571 | 98 | 837 |
| 78 | 584 | 99 | 850 |
| 79 | 597 | 100 | 862 |
| 80 | 610 | 101 | 875 |
| 81 | 622 | 102 | 888 |
| 82 | 635 | 103 | 900 |
| 83 | 647 | 104 | 913 |
| 84 | 660 | 105 | 926 |
| 85 | 672 |
AThe above hardness conversions cover an approximate relationship. The expected range of results on 95 % of hardness measurements is as follows:
Conversion from Vickers hardness to shore HFRSc scleroscope hardness, ±3.7 Shore.
Conversion from Shore HFRSc scleroscope hardness to Vickers hardness, ±43 HV.
BVickers hardness measurements are based on a load of 30 kgf. The Vickers penetrator was calibrated with a dead-weight Vickers hardness tester.